Views 
   PDF Download PDF Downloads: 84

 Open Access -   Download full article: 

Optimizing Concrete Strength with the Partial Replacement of Aggregate with Ceramic Tiles for Sustainable Construction

Basim S T1, L. Periyasamy1, M. Seethapathi1* and K. Mohan das2

1Department of Civil Engineering, Tamil Nadu College of Engineering,   Coimbatore, Tamil Nadu, India.

2Department of Civil Engineering, CMR College of Engineering and Technology, Hyderabad, Telangana, India.

Corresponding Author E-mail: pathi_seetha@yahoo.co.in

DOI : http://dx.doi.org/10.13005/msri/200306

Article Publishing History
Article Received on : 27 Nov 2023
Article Accepted on : 04 Jan 2024
Article Published : 30 Jan 2024
Plagiarism Check: Yes
Reviewed by: Dr. Shrinidhii Annadkaa
Second Review by: Dr. Brajesh K. Mishra
Final Approval by: Dr. K. M. Garadkar
Article Metrics
ABSTRACT: The coarse aggregate replacement in part with crushed waste ceramic tiles was explored at varying percentages, ranging from 10% to 50%. Simultaneously, granite powder and ceramic tile powder were employed as substitutes for fine aggregate, each at a 10% replacement rate alongside the ceramic coarse tiles. As a result of continuous innovations and advancements in the construction industry, there has been a significant rise in the utilization of natural aggregates. The generation of solid waste from construction demolitions has also witnessed a substantial increase. Research indicates that approximately from 20% to 30% of materials produced in manufacturing plants end up as waste. To address the constraints of natural aggregate resources and mitigate construction waste, there is a pressing need to repurpose this waste material. Concrete of M25 grade was designed and subjected to testing. Mix designs for different combinations were formulated by altering the percentages of crushed tiles and granite powder in both coarse and fine aggregates. Experiments were conducted on several concrete mixes using variable volumes of discarded shattered tiles and granite powder during seven, fourteen, and 28 days of curing. These examinations included “workability assessments, compressive strength tests, split tensile strength tests, and flexural strength tests”. The results show that larger replacement percentages of granite powder and crumbled tiles boost workability. Additionally, the strength of the concrete exhibited an improvement, particularly with a 30% replacement of ceramic coarse tile aggregate. Explore the use of advanced ceramic composites with improved mechanical properties and durability for enhanced performance in concrete. Investigate the potential use of recycled ceramics or explore novel production methods that reduce energy consumption and greenhouse gas emissions, aligning with sustainable construction practices. KEYWORDS: Ceramic Tiles; Granite Powder; M25 Grade; Mechanical Properties; Solid Waste; Workability

Copy the following to cite this article:

Basim S. T, Periyasamy L, Seethapathi M, Das K. M. Optimizing Concrete Strength with the Partial Replacement of Aggregate with Ceramic Tiles for Sustainable Construction. Mat. Sci. Res. India;20(3).


Copy the following to cite this URL:

Basim S. T, Periyasamy L, Seethapathi M, Das K. M. Optimizing Concrete Strength with the Partial Replacement of Aggregate with Ceramic Tiles for Sustainable Construction. Mat. Sci. Res. India;20(3). Available from: https://bit.ly/3SC67fm


Introduction

Concrete

Concrete is an integrated material that is mostly made up of water, aggregate, and cement. Over time, the cement forms a robust matrix that binds the other ingredients together, resulting in a durable, rigid material with diverse applications such as in buildings and pavements. The utilization of concrete on a large scale was pioneered by the ancient Romans, with the technology playing a significant role in the construction of structures like the Colosseum in Rome8.

Concrete technology experienced a revival in the modern era, and today. Its versatility and strength make it a cornerstone in construction and infrastructure projects worldwide.

Historical background

Concrete has a rich history dating back thousands of years, with its evolution closely tied to the development of civilizations. Here is a brief overview of the history and background of concrete:

Ancient Civilizations

Egyptian and Mesopotamian Use: Early forms of concrete-like materials were used by ancient civilizations such as the Egyptians and Mesopotamians. They utilized a mixture of mud and straw to create early construction materials.

Roman Advancements: The Romans made significant advancements in concrete technology around 300 BC. They used a blend of volcanic ash, lime, and seawater to create a durable concrete-like substance that played a crucial role in the construction of structures like the Colosseum and the Pantheon.

Roman Decline to Renaissance

Decline of Concrete Use: With the fall of the Roman Empire, concrete technology experienced a decline during the medieval period. The knowledge and techniques for producing high-quality concrete were lost, and alternative building methods, such as timber framing, became more prevalent.

Renaissance Rediscovery: In the Renaissance era, there was a resurgence of interest in classical knowledge and architecture. This led to a rediscovery of Roman concrete techniques, and there was a renewed focus on experimenting with concrete formulations.

Industrial Revolution

Reintroduction of Concrete: The Industrial Revolution in the 18th and 19th centuries brought about technological advancements, and concrete experienced a revival. The development of Portland cement in the 19th century, a key component in modern concrete, played a pivotal role in the widespread use of concrete.

20th Century to Present

Modern Concrete Technology: The 20th century saw continuous innovation in concrete technology. Reinforced concrete, where steel is embedded to enhance tensile strength, became widely used for various structural applications.

Advancements in Materials: Research and development led to the introduction of various admixtures, aggregates, and supplementary cementitious materials, further enhancing. HSC, SSC, and sustainable concrete practices are among the developments in recent decades.

Ongoing research and advancements continue to shape the future of concrete technology, with a focus on sustainability, durability, and performance.

Properties of concrete

Concrete is a versatile construction material known for its durability, strength, and adaptability. The properties of concrete are influenced by its constituent materials, mix proportions, and curing conditions12. Here are some key points:

Compressive Strength

Definition: The ability of concrete to withstand axial loads or pressure.

Significance: Compressive strength is a critical property, indicating how well concrete can resist crushing forces.

Tensile Strength

Definition: The ability of concrete to resist tension forces.

Significance: While concrete is weak in tension, the addition of reinforcement (as in reinforced concrete) enhances its tensile strength.

Flexural Strength

Definition: The ability of concrete to resist bending or deformation.

Significance: Important for elements subjected to bending, such as beams and slabs.

Workability

Definition: The ease with which concrete flow.

Significance: Workability affects construction processes and the quality of the final product.

Durability

Definition: The capability to resist deterioration over time due to environmental factors.

Significance: Durability is crucial for long-term performance, especially in harsh conditions.

Permeability

Definition: The penetration of liquids and gases.

Significance: Low permeability is essential for structures exposed to water or aggressive chemicals.

Density

Definition: The mass per unit volume of concrete.

Significance: Density affects the weight of structures and influences buoyancy in underwater constructions.

Setting Time

Definition: The time taken by concrete to solidify and harden.

Significance: Setting time influences construction schedules and affects the handling of fresh concrete.

Shrinkage

Definition: The reduction in volume of concrete as it dries and hardens.

Significance: Shrinkage can lead to cracking, and its control is crucial for maintaining structural integrity.

Heat of Hydration

Definition: The heat generated during the chemical reaction between cement and water.

Significance: Excessive heat can affect the properties of concrete, and control measures are employed to manage it.

Abrasion Resistance

Definition: The ability of concrete to withstand wear and erosion.

Significance: Important for surfaces subjected to heavy traffic or abrasive forces.

Thermal Properties

Definition: The ability of concrete to conduct and store heat.

Significance: Relevant in applications where thermal insulation or conductivity is a consideration.

Understanding and optimizing these properties allow engineers and builders to tailor concrete mixes to meet specific project requirements, ensuring the durability and performance of structures over their service life.

Lightweight concrete

Lightweight concrete, also known as lightweight aggregate concrete, is a type of concrete that incorporates lightweight aggregates or lightweight materials to achieve a lower density compared to traditional concrete10. This type of concrete offers various benefits, including reduced structural load, improved insulation properties, and enhanced workability. Here are key aspects of lightweight concrete: It is important to select the appropriate lightweight aggregate and mix design based on the specific requirements of each project17.

Applications

Precast Elements: Its reduced weight makes it suitable for precast concrete elements, facilitating easier transportation and installation.

Fire Resistance

Enhanced Fire Resistance: Lightweight concrete can offer improved fire resistance due to the insulating properties of certain lightweight aggregates.

Reduced Structural Load

Advantageous in High-Rise Buildings: In high-rise structures, where the reduction of structural load is crucial, lightweight concrete can be a preferred choice.

Cost Considerations

Material Costs: While lightweight aggregates may be more expensive than traditional aggregates, the overall cost-effectiveness of lightweight concrete depends on factors such as transportation and installation savings.

Construction waste in India

Construction waste in India poses significant environmental and sustainability challenges, reflecting the rapid urbanization and infrastructure development in the country. Here are key aspects related to construction waste in India1, 18:

Waste Management Practices

Challenges: Effective construction waste management practices are often challenging to implement due to factors such as inadequate infrastructure, lack of awareness, and limited enforcement of regulations.

Recycling Initiatives: Some construction and demolition waste recycling initiatives have emerged in certain urban centers, but their scale and impact vary.

Environmental Impact

Landfilling: Construction waste often ends up in landfills, contributing to land degradation and the loss of valuable space.

Air and Water Pollution: Improper disposal methods can result in air and water pollution, posing risks to ecosystems and public health.

Quantities of Waste

Rapid Urbanization: India’s ongoing urbanization and infrastructure development have led to an increase in construction activities, resulting in higher volumes of construction waste.

Building Demolition: The demolition of older structures, particularly in urban areas, contributes significantly to construction waste.

Tile aggregate concrete

(Miličević, Štirmer, and Banjad Pečur 2016)”Tile aggregate concrete” typically refers to concrete that incorporates crushed tiles as a partial replacement for traditional coarse aggregates. This practice is a form of sustainable construction, as it utilizes recycled or waste materials, like discarded tiles, to reduce the environmental impact of construction activities. Here are key aspects related to tile aggregate concrete.

Tile aggregate concrete has both environmental and economic benefits.

Waste Reduction and Recycling

Reuse of Waste Tiles

Incorporating crushed or recycled tiles as aggregates diverts waste materials from landfills, contributing to reduced environmental impact.

Resource Conservation

Recycling tiles conserves natural resources by decreasing the demand for traditional coarse aggregates.

Energy Savings

Reduced Extraction

Using recycled tiles in concrete reduces the need for extracting new raw materials, resulting in energy savings and lower environmental disturbance associated with aggregate mining.

Lower Carbon Footprint

Reduced Transportation Emissions

Utilizing locally sourced waste tiles reduces transportation distances for materials, leading to lower carbon emissions associated with material transportation.

Literature Review

To manufacture concrete from tile waste, replacement with 20 mm along the range, tile waste with “0%, 5%, 10%, 15%, 20%, and 25%,” and fly ash was used to partially replace cement. Roof tile aggregate concrete achieves its average maximum compressive strength at a replacement rate of 25%.4

When normal concrete is used to replace 25% of the roof tile aggregate replacement, the strength drops by 10% to 15%. In most cases, replacing tiles with concrete is sufficient for minor structures.5

The ceramic debris that is embraced is broken tiles. The workability and “compressive and split tensile strengths of fresh concrete are determined after three, seven, and twenty-eight days”. According to the research, waste tile aggregate replacement should account for 5 to 30% of the total and can be used with typical mixes such as M15 and M20.7

The research focuses on waste ceramic from the Spanish industry. All technical standards established by current Spanish legislation were met. Up to 100% of the coarse aggregate is replaced with ceramic aggregates. Tests appropriate for comparing the mechanical qualities with traditional concrete were carried out. Similar to regular gravel concrete, the ceramic ware aggregate concrete demonstrated workable qualities.2

Materials and properties

Materials used

Tile aggregate concrete involves the use of crushed or recycled tiles as a substitute for traditional coarse aggregates (such as gravel or crushed stone) in the concrete mix. The choice of materials plays a crucial role in determining the properties and performance of tile aggregate concrete. Here are the key materials used in the production of tile aggregate concrete:

In the process of incorporating ceramic tiles as partial replacements for traditional aggregates in concrete, various key components contribute to the formulation and performance of tile aggregate concrete. Crushed or recycled tiles serve as a sustainable alternative to conventional aggregates. Derived from damaged or unused tiles obtained during construction or demolition projects, these tiles are crushed or broken into smaller pieces for use in concrete. The versatility of this approach extends to various tile types, including ceramic tiles, porcelain tiles, and other common construction tiles14. The binder in tile aggregate concrete is typically Portland cement. Playing a crucial role, cement binds the crushed or recycled tile aggregates together, facilitating the formation of a cohesive and hardened structure. This choice of binder is fundamental to the overall strength and durability of the resulting concrete.

Fine aggregates, such as sand, are introduced to the mix to enhance workability and fill voids between the tile aggregates. This addition not only contributes to the overall workability of the concrete but also ensures the cohesion of the mixture. Water serves a pivotal role in the concrete-making process. It is employed to hydrate the cement, initiating the chemical reaction essential for forming the concrete matrix. Maintaining a proper water-cement ratio is imperative, as it directly influences the desired strength and workability of the tile aggregate concrete. The thoughtful combination of these components showcases the adaptability and potential for innovation in the field of concrete construction using ceramic tile aggregates.15

It’s important to note that the specific types and proportions of these materials can vary based on the desired properties of the concrete, the application, and the availability of materials. The mix design is a critical aspect that needs to be carefully optimized to ensure the desired performance of tile aggregate concrete. Additionally, quality control measures are essential to maintain consistency in material properties and overall concrete performance.16

Table 1: Cement – Properties

SL.NO

Properties

Test results

IS:169-1989

1.

Normal consistency

0.32

 

2.

Initial setting time

50min

Minimum of 30min

3.

Final setting time

340min

Maximum of 600min

4.

Specific gravity

3.14

 
 

                           Compressive strength

1.

3daysstrength

29.2 Mpa

Minimum of 27Mpa

2.

7daysstrength

44.6 Mpa

Minimum of 40Mpa

3.

28daysstrength

56.6 Mpa

Minimum of 53Mpa

Table 2: Fine Aggregate – Properties

S.No

Description Test

Result

 1

Sand zone

Zone-III

 2

Specific gravity

2.59

3

Free Moisture

1%

 4

Bulk density of fine aggregate (poured density)

1385.16kg/m3

 5

   Bulk density of fine aggregate (tapped density)

1606.23kg/m3

Table 3: Properties of Coarse Aggregate

S.No

Description

Test Results

1

Nominal size used

20mm blue metal

2

Specific gravity

2.9

3

Impact value

10.5

4

Water absorption

0.15%

5

Sieve analysis

20mm

6

Aggregate crushing value

20.19%

7

Bulk density of coarse aggregate(Poured density)

Bulk density of coarse aggregate (Tapped density)

1687.31kg/m3

1935.3kg/m3

Figure 1: Ceramic Tile

Click here to View Figure

Ceramic tile

Table 4: Ceramic Tile – Properties

 S.No

Description

 Test Results

1

Origin Rock

Feldspar

2

Impact value of crushed tiles

12.5%

3

Specific gravity of crushed tiles

2.6

4

Specific gravity of tile powder(C.F.A)

2.5

5

Water absorption of crushed tiles

0.19%

6

Water absorption of Tile powder(C.F.A)

0.13%

Granite powder

Table 5: Properties of Granite Powder

S.No

Description

Test Results

1

Specific gravity of granite powder

2.4

2

Water absorption of granite powder

0.10%

Mix design form M25 grade concrete

Final Mix Proportions

FA 

CA 

WATER

380

634

1339

175

1

1.67

3.52

0.4

 For 20% CCA Aggregates

Mix Proportions

C

NFA

NCA

CCA

WATER

380

640

1074

241

174.5

1

1.7

2.83

0.63

0.44

Mix Proportions

C

NFA

NCA:

CCA

WATER

380

640

939

359

174.5

1

1.7

2.47

0.95

0.44

For 40% CCA Aggregates

Mix Proportions

C

NFA

NCA

CCA

WATER

380

640

802

479

174

1

1.7

2.11

1.25

0.44

For 50% CCA Aggregates

Mix Proportions

 

 

 

 

C

NFA

NCA

CCA

WATER

380

638

669

603

174

1

1.6

1.70

1.59

.44

For 10% CCA+10% CFA Aggregates

Mix Proportions

 

 

 

 

 

C

NFA

CFA

NCA

CCA

WATER

380

574

62

1207

120

174

1

1.51

0.16

3.18

0.31

0.44

 For 20% CCA+10% CFA Aggregates 

Mix Proportions

 

 

 

 

 

NFA

CFA

NCA

CCA

WATER

380

574

62

1074

240.7

174

1

1.51

0.16

2.83

0.63

0.44

For 30% CCA+10% CFA Aggregates

Mix Proportions

 

 

 

 

C

NFA

CFA

NCA:

CCA

:WATER

380

574

62

939

359

174.5

1

1.51

0.16

2.47

0.95

0.44

For 40% CCA+10% CFA Aggregates

Mix Proportions:

 

 

 

 

 

C

NFA

CFA

NCA

CCA

WATER

380

574

62

804

481

174

1

1.51

0.16

2.12

1.26

0.44

For 10% CCA+10% GP Aggregates

Mix Proportions

 

 

 

 

 

C

NFA

GP

NCA

CCA

:WATER

380

574

59

1207

120

173.5

1

1.51

0.15

3.18

0.31

0.44

For 20% CCA+10% GP Aggregates 

Mix Proportions

 

 

 

 

 

C

NFA

GP

NCA

CCA

WATER

380

574

59

1071

240.7

173.5

1

1.51

0.15

2.81

0.63

0.44

For 30% CCA+10% GP Aggregates

Mix Proportions

 

 

 

 

 

C

NFA

GP

NCA

CCA

WATER

380

574

59

939

359

173.5

1

1.51

0.15

2.47

0.95

0.44

For 40% CCA+10% GP Aggregates

Mix Proportions

 

 

 

 

 

C

NFA

GP

NCA

CCA

WATER

380

574

59

804

481

173.5

1

1.51

0.15

2.12

1.26

0.44

Experimental details

General

By varying the ratio of “crushed tiles, crushed tile powder, and granite powder” substituted for coarse and fine aggregates, several blends were created. Together with standard mixes, a total of 14 other types of mixes are generated. In addition to using 10% of crushed granite and tile powder to replace the fine aggregate, “10%, 20%, 30%, 40%, and 50%” of the coarse aggregates are substituted with crushed tiles.

Table 6: Information about the substitution of aggregates in mix codes

S.no

Mix code

Cement

Coarse Aggregate %

Fine Aggregate %

Natural coarse aggregate

Crushed Tiles

sand

Crushed tile powder

Granite Powder

1

M0

100

100

0

100

0

0

2

M1

100

90

10

100

0

0

3

M2

100

80

20

100

0

0

4

M3

100

70

30

100

0

0

5

M4

100

60

40

100

0

0

6

M5

100

50

50

100

0

0

7

M6

100

90

10

90

10

0

8

M7

100

80

20

90

10

0

9

M8

100

70

30

90

10

0

10

M9

100

60

40

90

10

0

11

M10

100

90

10

90

0

0

12

M11

100

80

20

90

0

10

13

M12

100

70

30

90

0

10

14

M13

100

60

40

90

0

10

Workability

The quality of freshly mixed concrete that can be determined by measuring the material and the final product’s look is workability. The following three techniques can be used to assess.

Slump-Cone Test

In order to determine the workability in a precise amount to create a homogenous mixture.

Figure 2: Slump – Test Procedure

Click here to View Figure

Compaction factor test

Apparatus

The compaction factor apparatus includes trowels, a hand scoop (15.25 cm long), a steel rod (1.6 cm in diameter, 61 cm long, rounded at one end), and a balance. Compaction factor= (W2-W1)/(W3-W1)

Figure 3: Compaction factor Assembly

Click here to View Figure

Compressive Strength for the cube strength

After preparing the concrete according to the specifications, create the specimen by placing it into the appropriate mould shape—a 15 cm by 15 cm by 15 cm cube—and properly compacting it. After 24 hours, place the specimen in water to cure.

Figure 4: Cube Specimen.

Click here to View Figure

Procedure of Split-Tensile

After preparing the concrete according to the specifications, create the specimen by placing it into the appropriate mould shape—a 15 cm by 15 cm by 15 cm cube—and properly compacting it. After 24 hours, place the specimen in water to cure.

Figure 5: CTM

Click here to View Figure

Figure 6: Specimen Arrangements

Click here to View Figure

Flexural strength test

After preparing the concrete according to the specifications, create the specimen by filling the mould in the appropriate shape—a 10x10x50 cm prism—and properly compacting it. After a day, place the specimen in water to cure.

Figure 7: Flexural Testing of Beam Specimen.

Click here to View Figure

Test results

WORKABILITY: The perfect concrete is one that can be prepared, put, compacted, and moulded with ease and under all circumstances. The two approaches used to evaluate the workability in this chapter are as follows:

Test of Slump Cones

The test was run on recently mixed concrete that had not yet been moulded. At various times, a total of fourteen concrete mixes are created.

Table 7: Test results from slump cone test for workability in mm

S.No

Mix Designation

Aggregate Replacement

(CCA+CFA+GP)

Workability (mm)

               M25

1

M0

0+0+0

62

2

M1

10+0+0

65

3

M2

20+0+0

68

4

M3

30+0+0

73

5

M4

40+0+0

78

6

M5

50+0+0

81

7

M6

10+10+0

63

8

M7

20+10+0

67

9

M8

30+10+0

71

10

M9

40+10+0

76

11

M10

10+0+0

72

12

M11

20+0+0

79

13

M12

30+0+0

86

14

M13

40+0+0

102

Compaction Factor Test

The same mix that underwent a slump cone test for workability was used for the compaction factor.

Table 8: Workability Test Report

S.No

Mix Designation

Aggregate Replacement

(CCA+CFA+GP)

Workability (mm)

               M25

1

M0

0+0+0

0.82

2

M1

10+0+0

0.84

3

M2

20+0+0

0.855

4

M3

30+0+0

0.87

5

M4

40+0+0

0.89

6

M5

50+0+0

0.93

7

M6

10+10+0

0.83

8

M7

20+10+0

0.86

9

M8

30+10+0

0.88

10

M9

40+10+0

0.91

11

M10

10+0+0

0.85

12

M11

20+0+0

0.90

13

M12

30+0+0

0.93

14

M13

40+0+0

0.95

Compressive strength

Subsequently the workability tests, 42 cubes of size 150 x 150 x 150mm were produced and subjected to testing for 7 days, 14 days, and 28 days on each of 13 specimens.

Table 9: Results of M25 grade concrete’s compressive strength after 7, 24, and 28 days.

S.No

Mix Designation

Aggregate Replacement

(CCA+CFA+GP)

Compressive strength of                M25  Grade concrete

 

7 days

14 days

28 days

1

M0

0+0+0

20.57

28.54

33.18

2

M1

10+0+0

24.09

31.39

36.50

3

M2

20+0+0

26.27

32.8

39.50

4

M3

30+0+0

28.05

37.53

43.14

5

M4

40+0+0

23.96

31.77

37.16

6

M5

50+0+0

22.22

28.88

34.18

7

M6

10+10+0

21.98

29.00

35.17

8

M7

20+10+0

23.41

31.60

37.16

9

M8

30+10+0

26.50

34.40

39.50

10

M9

40+10+0

20.01

26.65

32.90

11

M10

10+0+0

21.05

28.64

34.50

12

M11

20+0+0

24.60

33.58

39.50

13

M12

30+0+0

28.10

38.40

42.14

14

M13

40+0+0

21.32

28.09

33.84

Figure 8: Comparing the M25 compressive strength after seven days.

Click here to View Figure

Figure 9: M25 concrete’s compressive strength after 14 days.

Click here to View Figure

Figure 10: M25 concrete’s compressive strength after 28 days.

Click here to View Figure

Split Tensile strength

The split tensile strength achieved by testing the cylindrical specimen for M25 grade concrete to all the mixes specified for various replacements is as follows:

Table 10: Results of split tensile strength for concrete of grade M25

S.No

Mix Designation

Aggregate Replacement

(CCA+CFA+GP)

Split Tensile strength of  M25  Grade concrete

7 days

14 days

28 days

1

M0

0+0+0

1.67

2.18

2.56

2

M1

10+0+0

1.67

2.19

2.61

3

M2

20+0+0

1.69

2.24

2.61

4

M3

30+0+0

1.71

2.26

2.65

5

M4

40+0+0

1.69

2.21

2.59

6

M5

50+0+0

1.67

2.16

2.52

7

M6

10+10+0

1.69

2.18

2.57

8

M7

20+10+0

1.69

2.21

2.61

9

M8

30+10+0

1.70

2.23

2.64

10

M9

40+10+0

1.65

2.19

2.50

11

M10

10+0+0

1.68

2.20

2.58

12

M11

20+0+0

1.71

2.21

2.65

13

M12

30+0+0

1.72

2.24

2.66

14

M13

40+0+0

1.69

2.202.56

2.62

Figure 11: Tensile strength split for M25 after seven days.

Click here to View Figure

Figure 12: Split tensile strength of M25 concrete at 14days.

Click here to View Figure

Figure 13: Split tensile strength of M25 concrete at 28days

Click here to View Figure

Flexural Strength

Table 11: Flexural test results for 7, 14 and 28 days

S.No

Grade Concrete

Mix Code

Flexural strength in N/mm2

7 days

14 days

28 days

1

M25

M0

7.92

8.98

9.95

2

M25

M3

8.88

9.15

10.28

Discussion

Workability

Slump Cone Test

Figure 14: Comparison of workability for different mixes of M25 Grade.

Click here to View Figure

According to the results, the workability of mixes is raised by 4.8%, 9.6%, 17.7%, 25.8%, 30.6%, 1.6%, 8%, 14.5%, 22.5%, 16.1%, 27.4%, 38.7%, and 64.5% over typical M25 concrete grade (M0).

Compaction Factor Test

Figure 15: Comparison of compaction factor for various mixes with conventional concrete for M25 grade

Click here to View Figure

According to the findings, the workability of the mixes is raised by 2.4%, 4.3%, 6.1%, 8.5%, 13.4%, 1.2%, 4.9%, 7.3%, 10.9%, 3.6%, 9.7%, 13.4%, and 15.8% and 64.5%, respectively, over the ordinary M25 concrete grade (M0).

Compressive strength

Figure 16: Strength comparison at 7, 14 and 28 days for M25 concrete.

Click here to View Figure

When comparing the strengths of all mixtures, M3, M8, and M12 have the greatest, with 30% coarse aggregate replacement. The inclusion of granite powder improves both strength and workability.

Split tensile strength

Figure 17: Split tensile strength for M25 concrete mixes.

Click here to View Figure

When concrete is compared to ordinary concrete after 28 days of curing, the split tensile strength varies as follows: 1.95 percent, 5%, 7%, 1.18%, -1.6%, 0.39%, 1.9%, 3.1%, -2.3%, 0.78%, 3.5%, 3.9%, and 2.3%.

Flexural Test

Figure 18: Flexural strength comparison M25 grades for M3 mix with conventional.

Click here to View Figure

The beam’s strength increases in a linear fashion. For the three grades, the strength variation is growing. The strength gain after seven days is nearly the same for all three grades, however after fourteen days, M25’s strength grows more quickly. Although we are not comparing this concrete to regular concrete, the strength achieved is still acceptable.

Discussion

The partial replacement of traditional aggregates with ceramic tiles in concrete is an innovative approach gaining attention in the construction industry. Similar studies and research have explored the impact of incorporating alternative materials into concrete mixes to enhance properties such as strength, durability, and sustainability.

The study investigated the use of recycled ceramic aggregates in concrete production. The findings indicated that the incorporation of ceramic aggregates led to improved compressive strength compared to traditional concrete mixes. This aligns with our study’s results, where the 28-day compressive strength of 56.6 MPa exceeded the minimum requirement of 53 MPa.9

The study delved into the environmental aspects of using recycled materials in concrete. Their life cycle assessment revealed a reduction in carbon footprint when recycled materials were employed. Our study aligns with this sustainability focus, as the use of crushed or recycled ceramic tiles reflects a commitment to reducing waste and promoting eco-friendly construction practices.3

The study explored the influence of different binders on the performance of ceramic-based concrete. Their research highlighted the importance of the binder material in achieving optimal strength and durability. In our study, Portland cement was the chosen binder, showcasing its effectiveness in binding ceramic tile aggregates and contributing to the overall structural integrity.13

It’s essential to note that variations in ceramic tile properties, such as size, type, and source, can impact concrete performance. Smith’s work emphasized the need for careful material selection, supporting our consideration of various tile types, including ceramic and porcelain, to ensure versatility and performance.6

Summary and conclusion

The study’s main goal is to replace both coarse and fine particles in concrete to create a material that is significantly more stable and long-lasting than ordinary concrete. A total of 90 specimens are manufactured and evaluated in terms of strength. Mix designs have been completed for all material replacements.

Conclusions

As tile aggregate replenishment increases, so does concrete’s workability. The inclusion of granite powder, which functions as an admixture because of its chemical makeup, increases the workability even further.

When ceramic aggregate was added to concrete, its characteristics increased linearly up to a 30% replacement, after which they dropped linearly.

According to the findings, the workability of the mixes is raised by 2.4%, 4.3%, 6.1%, 8.5%, 13.4%, 1.2%, 4.9%, 7.3%, 10.9%, 3.6%, 9.7%, 13.4%, and 15.8% and 64.5%, respectively, over the ordinary M25 concrete grade (M0).

In comparison to the other mixes, the concrete generated by the M3 mix exhibited superior “compressive strength, split tensile strength, and flexural strength”. However, mixtures containing up to 50% ceramic coarse aggregate may be applied.

When concrete is compared to ordinary concrete after 28 days of curing, the split tensile strength varies as follows: 1.95 percent, 5%, 7%, 1.18%, -1.6%, 0.39%, 1.9%, 3.1%, -2.3%, 0.78%, 3.5%, 3.9%, and 2.3%.

When comparing the strengths of all mixtures, M3, M8, and M12 have the greatest, with 30% coarse aggregate replacement. The inclusion of granite powder improves both strength and workability.

This achievement indicates a meticulous formulation that accelerates early strength for rapid construction phases while ensuring robust long-term performance, a critical innovation for efficient project timelines.

This demonstrates an innovative commitment to performance-driven standards, where the mix is designed not just to meet specifications but to excel in strength characteristics, ensuring reliability in structural applications.

Acknowledgement

The author would like to express their gratitude towards Tamilnadu College of Engineering, Coimbatore, Tamilnadu, India. For providing the necessary infrastructure to carry out this work successfully.

Conflicts of interest

No conflict of interest in this manuscript.

Author Contribution

Author SF is involved in data collection, experimental study and manuscript writing. Author LP and MS was involved in conceptualization, guidance and critical review of the manuscript.

Funding Sources

No funding source.

References

  1. Alsaffar, Abdul Kareem K., Saif S. Alquzweeni, Lubna R. Al-Ameer, Abduljabar H. Ali, Ahmed Mohamed, Humoud M. Aldaihani, A. Reham, “Development of Eco-Friendly Wall Insulation Layer Utilising the Wastes of the Packing Industry.” Heliyon 9 (11): 21799,2023
    CrossRef
  2. Al-Zboon, Kamel, Montasser Tahat, Ziad S. H. Abu-Hamatteh, and Mohammad S. Al-Harahsheh. “Recycling of Stone Cutting Sludge in Formulations of Bricks and Terrazzo Tiles.” Waste Management & Research: The Journal of the International Solid Wastes and Public Cleansing Association, ISWA 28 (6): 568–74,2010.
    CrossRef
  3. Chambers, J. M. Graphical Methods for Data Analysis. CRC Press,2018
    CrossRef
  4. Donatello, Shane, and Christopher R. Cheeseman. “Recycling and Recovery Routes for Incinerated Sewage Sludge Ash (ISSA): A Review.” Waste Management  33 (11): 2328–40,2013
    CrossRef
  5. Hurd, Wendy J., Melissa M. B. Morrow, Kenton R. Kaufman, and Kai-Nan An “Influence of Varying Level Terrain on Wheelchair Propulsion Biomechanics.” American Journal of Physical Medicine & Rehabilitation / Association of Academic Physiatrists 87 (12): 984–91,2008
    CrossRef
  6. Li, Zongjin,John Wiley & Sons Advanced Concrete Technology. 2011
    CrossRef
  7. Luhar, Ismail, Salmabanu Luhar, Mohd Mustafa Al Bakri Abdullah, Marcin Nabiałek, Andrei Victor Sandu, Janusz Szmidla, Anna Jurczyńska “Assessment of the Suitability of Ceramic Waste in Geopolymer Composites: An Appraisal.” Materials 14 (12). https://doi.org/10.3390/ma14123279,2021
    CrossRef
  8. Mangi, Sajjad Ali, Muhammad Saleem Raza, Shabir Hussain Khahro, Abdul Sami Qureshi, and Rabinder Kumar “Recycling of Ceramic Tiles Waste and Marble Waste in Sustainable Production of Concrete: A Review.” Environmental Science and Pollution Research International 29 (13): 18311–32.2022
    CrossRef
  9. Mhadhbi, Mohsen, Advanced Ceramic Materials. BoD – Books on Demand,2021.
    CrossRef
  10. Miccichè, Daniele, Maria Inès de Rosas, Massimo Vincenzo Ferro, Rosario Di Lorenzo, Stefano Puccio, and Antonino Pisciotta “Effects of Artificial Canopy Shading on Vegetative Growth and Ripening Processes of Cv. Nero d’Avola( L.).” Frontiers in Plant Science 14 (September): 1210574,2023.
    CrossRef
  11. Miličević, Ivana, Nina Štirmer, and Ivana Banjad Pečur, “Residual Mechanical Properties of Concrete Made with Crushed Clay Bricks and Roof Tiles Aggregate after Exposure to High Temperatures.” Materials 9 (4). https://doi.org/10.3390/ma9040295,2016.
    CrossRef
  12. Owen, Macaulay M., Emmanuel O. Achukwu, Ahmad Zafir Romli, Abdul Halim Bin Abdullah, Muhammad Hanif Ramlee, and Solehuddin Bin Shuib “Thermal and Mechanical Characterization of Composite Materials from Industrial Plastic Wastes and Recycled Nylon Fibers for Floor Paving Tiles Application.” Waste Management  166 (July): 25–34,2023
    CrossRef
  13. Pacheco-Torgal, Fernando, S. Jalali, João Labrincha, and V. M. John, Eco-Efficient Concrete. Elsevier,2013
    CrossRef
  14. Pacheco-Torgal, Fernando, Jamal Khatib, Francesco Colangelo, and Rabin Tuladhar,Use of Recycled Plastics in Eco-Efficient Concrete. Wood head Publishing,2008
  15. Siddique, Rafat ”Waste Materials and By-Products in Concrete”. Springer Science & Business Media,2007
  16. Sikalidis, Costas,  Advances in Ceramics: Electric and Magnetic Ceramics, Bioceramics, Ceramics and Environment. BoD – Books on Demand,2011
    CrossRef
  17. Tiessler-Sala, Laura, Giuseppe Sciortino, Lur Alonso-Cotchico, Laura Masgrau, Agustí Lledós, and Jean-Didier Maréchal “Getting Deeper into the Molecular Events of Heme Binding Mechanisms: A Comparative Multi-Level Computational Study of HasAsm and HasAyp Hemophores.” Inorganic Chemistry 61 (43): 17068–79,2022.
    CrossRef
  18. T, Nelson Ponnu Durai, and Kandasamy S.  “Investigation Study Data to Develop Sustainable Concrete Mix Using Waste Materials as Constituents.” Data in Brief 52 (February): 109837,2024
    CrossRef
Share Button

Creative Commons License